Sample Preparation for Molecular Weight measurements on the Zetasizer Nano and μV

This note summarizes the preparation of samples for the measurement of absolute molecular weight using static light scattering on the Zetasizer Nano and μV instruments using a polystyrene molecular weight standard sample as an example

Introduction

This technical note summarizes the preparation of samples suitable for the measurement of absolute molecular weight using static light scattering on the Zetasizer Nano and µV instruments. It uses a polystyrene molecular weight standard sample as an example of the procedures involved to obtain suitable samples for successful molecular weight measurements. However, other suitable samples can be prepared using the guidelines contained in this document.

Experimental

Materials

  • A suitable polystyrene molecular weight standard of around 200,000 g/mol.
  • Toluene (CHROMASOLV® HPLC grade).
  • Glass or quartz cuvettes with stoppers. Ideally these should be indexed matched to ensure that the scattering differences between cuvettes are negligible. For samples prepared in toluene, 4 cuvettes will be required (1 for toluene and 3 for the various sample concentrations). For samples prepared in other solvents, 5 cuvettes will be required (1 for toluene, 1 for the solvent and 3 for the various sample concentrations).
  • Suitable filters and syringes for filtration of toluene into the cuvettes.

Method

Table 1: Guidelines for the preparation of appropriate concentrations of polystyrene molecular weight standard
Weight of Polystyrene Molecular Weight Standard (mg)Weight of Toluene (g)Final Sample Concentration (mg/mL)
1.52.60.499
32.60.998
4.52.61.497

Prepare 3 different concentrations of the polystyrene molecular weight standard in toluene by accurately weighing appropriate amounts of powder and toluene into the cuvettes and stopper them to prevent any solvent evaporation. It is easier to weigh toluene and use its density value of 0.865kg/m³) to calculate the volume of solvent used. Recommended sample concentrations to be prepared are 0.5, 1.0 and 1.5mg of polystyrene molecular weight standard per mL of toluene respectively. Guidelines for the preparation of appropriate concentrations of molecular weight standard are shown in table 1

Allow the samples to stand for 1 hour to ensure complete solubilization of the polymer in the solvent.

Perform a sizing measurement on each concentration to check for modality and the presence of any dust or aggregates. Ideally, the sample should consist of a single peak. If not, the sample needs to be prepared again. Measure the various sample concentrations using DLS to check if dilution influences the size.

If the sample quality is good then a molecular weight measurement can be performed.

Use the "Polystyrene in toluene molecular weight.sop" supplied with the Zetasizer software to measure the samples.

Experimental Observations

The count rate traces obtained should be fluctuating with time over a narrow range of intensity values. This is indicative of a sample free of large particles, aggregates or dust. Figure 1 shows a typical count rate trace of a suitable sample for molecular weight measurement.

Figure1: A typical count rate trace of a suitable sample for molecular weight measurement
MRK1832 fig1

"Spikes" in the count rate trace indicate the presence of dust and/or aggregates and will result in poor data quality and poor molecular weight results. Figure 2 shows a typical count rate trace obtained from a sample containing aggregates. If such data is obtained, the samples will need to be filtered and re-measured. Filtration of a sample will result in a loss of material and the correct concentration of the sample will need to be determined.

Figure 2: A typical count rate trace obtained from a sample containing aggregates
MRK1832 fig2

For protein samples, the measurement of the absorbance at a suitable wavelength will allow for concentration determination using the protein's extinction coefficient at that wavelength. For polymer solutions which are not chromophores, the determination of concentration is more difficult and a suitable refractometer is required.

Cycling of the count rate trace indicates that the sample is not thermally equilibrated (Figure 3). In such circumstances, a longer equilibration time should be defined in the SOP.

Figure 3: A typical count rate trace of a sample which is not thermally equilibrated
MRK1832 fig3

The intensity of scattered light obtained from each sample concentration should increase linearly. This can be checked from the Debye plot shown on the Molecular Weight report supplied with the Zetasizer software. If the intensity does not increase linearly with sample concentration, then the samples will need to be prepared again and the measurements redone.